4(Te,Sb) eutectic phase reduces continuously, the morphology of silicon particles change from pin-like, polygonal and long-rod to short-rod like, oval and spherical, the average size is merely 9 μm. The average tensile strength, yield strength, elongation, reduction of area and Vickers hardness after solidifing at 545℃ for 20h and aging at 170℃ for 10h with the polyethylene glycol quenching medium are 360MPa, 307MPa, 10.4%, 13.8% and 122, dimple morphology is the dominated fracture surface, accompanied by some intergranular fracture zone, and the average length of Mg2Si phase is about 224nm."/>
[fanzhenzhong, Wang Duanzhi, Wang Kunpeng, Xiong Yancai, Lu Zheng, Zheng Weidong. Study on Microstructure and Mechanical Properties of ZL114A Alloy in T6 State Bearing Te and Sb[J]. Rare Metal Materials and Engineering,2018,47(12):3880~3886.]