2 had the apparent effect in increasing the weld penetration, it was 2 times the depth of weld without flux. KF was in the second place. LiF could decrease the weld penetration; Compared with MgF2, KF had a small weld width , narrow HAZ width and total joint width. NaF obtained the minimum HAZ width; The angle of NaF, KF, MgF2 and AlF3 between columnar crystal growth direction and weld center axis was bigger than the other fluoride. The length of the column crystal size was determined by the size of penetration, the width variation law was for AlF3>KF>MgF2>NaF; the grain size of coarse grain area in HAZ was for MgF2 > NaF > AlF3 > KF."/>
[Gao Xiaogang, Dong Junhui, Han Xu. Effect of Different Fluoride on Weld Formation and Organization with A-TIG Welding of Titanium Alloy[J]. Rare Metal Materials and Engineering,2017,46(6):1638~1643.]